Bamboo gun nail and production method thereof

文档序号:1869562 发布日期:2021-11-23 浏览:15次 中文

阅读说明:本技术 竹枪钉及其生产方法 (Bamboo gun nail and production method thereof ) 是由 钱一辰 于 2021-07-27 设计创作,主要内容包括:本申请公开了一种竹枪钉及其生成方法,所述竹枪钉由多枚厚度与宽度相等的竹钉并联粘接成排而成,所述竹钉的钉头呈多边锲形或圆锥形,相邻两枚所述竹钉的钉体之间有胶粘剂隔开,所述竹钉的钉尾厚度大于所述钉体厚度,分别呈方形或长方形,所述竹钉为强化层与薄竹片层一一间隔的层状结构,密度大于1200kg/m~(3)。(The application discloses a bamboo gun nail and a generation method thereof, the bamboo gun nail is formed by parallelly bonding a plurality of bamboo nails with equal thickness and width in a row, and the nail heads of the bamboo nailsThe bamboo nail is in a polygonal wedge shape or a conical shape, the nail bodies of two adjacent bamboo nails are separated by adhesive, the thickness of the nail tail of each bamboo nail is larger than that of the nail body and is respectively square or rectangular, each bamboo nail is in a layered structure with a reinforcing layer and a thin bamboo sheet layer which are separated one by one, and the density of each bamboo nail is larger than 1200kg/m 3 。)

1. The bamboo gun nail is characterized by being formed by parallelly bonding a plurality of bamboo nails with the same thickness and width in rows, the nail heads (1) of the bamboo nails are in a polygonal wedge shape or a conical shape, the nail bodies (2) of two adjacent bamboo nails are separated by an adhesive, the thickness of the nail tails (3) of the bamboo nails is larger than that of the nail bodies (2) and is respectively square or rectangular, the bamboo nails are in a layered structure with a reinforcing layer (4) and a thin bamboo sheet layer (5) separated one by one, and the density of the bamboo nails is larger than 1200kg/m3

2. The method of producing bamboo nailers of claim 1 including:

(1) unit processing: rotary cutting the bamboo sections into bamboo sheets;

(2) and (3) drying: drying the bamboo slices in the step (1) by adopting a hot pressing plate until the water content is 3% -5%;

(3) strengthening: selecting an enhancer, and performing enhancement treatment on the bamboo sheet in the step (2) in an impregnation mode, wherein the solid content of the enhancer is 10% -15%, and the adhesion amount of the enhancer is more than 22%;

(4) and (3) drying: drying the bamboo slices in the step (3) by adopting a hot pressing plate until the water content is 1% -5%;

(5) assembling: superposing the bamboo sheets in the step (4) according to the same direction of the bamboo fibers, wherein the included angle of the bamboo fibers in different layers is 0-3.5 degrees, and assembling the bamboo sheets into a blank with a layered structure;

(6) molding: hot-pressing the blank in the step (5) in a hot press, wherein the pressure is 40-120Mpa, the temperature is determined by the curing temperature of a reinforcing agent, the hot-pressing time is 70-150s/mm, and the blank is pressed into a laminated reinforcing plate with the thickness of 2.0-10.0 mm;

(7) nail blank processing: storing the laminated board in the step (6) for more than 4h at normal temperature or in a temperature and humidity regulating room, and cutting the laminated board into nail blanks according to the length and the size of each processed gun nail;

(8) machining: milling and grinding two surfaces of the nail blank of (7) according to the thickness specification of the gun nail to enable the nail head to be wedge-shaped, extruding the end surface of the nail tail to form deep marks parallel to the surface, wherein the number of the deep marks is positively correlated with the thickness of the nail body, the number of the deep marks is at least 1, the deep marks are positioned on the thickness central plane or the symmetrical plane of the end surface of the nail tail, the depth of the deep marks is 0.5-2mm, the depth of the deep marks in the middle of the thickness is deep, the depth of the deep marks closer to the two surfaces is shallow, and the taper angle of the deep marks is 10-40 degrees;

(9) and (3) wrapping end processing: wrapping one end of the nail tail of the nail body (8) with a compression-resistant resin layer, wherein the thickness of the resin layer is 0.9-2.8mm, extruding the two sides of the resin layer into a dovetail shape in a mold, and then curing the resin layer into a trapezoid, wherein the thickness of the long side of the nail tail end after curing is 1.5-2.0 times of the thickness of the nail body;

(10) stripping and arranging: and finally, quickly bonding the strip gun nails in rows in a lateral direction, wherein the bonding area is 5-25% of the area of the side surface, and manufacturing the strip bamboo gun nails.

3. The method for producing bamboo gun nail according to claim 2, wherein the bamboo age of the bamboo segments is 5 to 8 years.

4. The method of producing bamboo nailers of claim 2 wherein the thickness of the bamboo sheet is 0.12 to 0.25 mm.

5. The method for producing bamboo gun nail according to claim 2, wherein the nail body has a thickness of 1 piece less than 3mm and 2-3 pieces more than 3 mm.

6. The method for producing bamboo gun nail according to claim 2, wherein the compression resistant resin is selected from epoxy resin or modified isocyanate.

7. The method of manufacturing bamboo nailers of claim 2 wherein said bamboo chips are within 1/3 inner bamboo wall thickness adjacent the outer bamboo green.

8. The method for producing bamboo nailers of claim 2 wherein the automatic rotary differential sander is a toothpick sander adjusted for orientation and sanding angle.

9. The method for producing bamboo gun nail according to claim 2, wherein the trapezoid angle is 50 ° to 75 °.

Technical Field

The application relates to the technical field of bamboo gun nails, in particular to a bamboo gun nail and a production method thereof.

Background

CN101158369A discloses a bamboo straight-row nail and a manufacturing method thereof, which provides a new method and means for high-quality application of bamboo, but the manufacturing parameters are not accurate enough, the production process time is long, the yield is low, and the problems of nail tail fuzzing, tearing between nails, insufficient stability in the striking process of the bamboo nail and the like occur in the use process.

Disclosure of Invention

The embodiment of the application aims to provide a bamboo gun nail and a production method thereof, and aims to solve the problems that the yield is low in the production process, nail tail fluffing occurs in the use process, the nails are torn, and the stability is insufficient in the bamboo nail striking process.

According to a first aspect of the embodiments of the present application, a bamboo nailer is provided, wherein the bamboo nailer is formed by a plurality of bamboo nails with equal thickness and width which are connected in parallel and bonded in rows, a nail head (1) of the bamboo nailer is in a polygonal wedge shape or a conical shape, nail bodies (2) of two adjacent bamboo nails are separated by an adhesive, a nail tail (3) of the bamboo nailer is thicker than the nail bodies (2) and is respectively in a square or rectangular shape, the bamboo nailer is in a layered structure with a reinforcing layer (4) and a thin bamboo sheet layer (5) separated one by one, and the density is higher than 1200kg/m3

According to a second aspect of embodiments of the present application, there is provided a method of producing a bamboo gun nail of the first aspect, comprising:

(1) unit processing: rotary cutting the bamboo sections into bamboo sheets;

(2) and (3) drying: drying the bamboo slices in the step (1) by adopting a hot pressing plate until the water content is 3% -5%;

(3) strengthening: selecting an enhancer, and performing enhancement treatment on the bamboo sheet in the step (2) in an impregnation mode, wherein the solid content of the enhancer is 10% -15%, and the adhesion amount of the enhancer is more than 22%;

(4) and (3) drying: drying the bamboo slices in the step (3) by adopting a hot pressing plate until the water content is 1% -5%;

(5) assembling: superposing the bamboo sheets in the step (4) according to the same direction of the bamboo fibers, wherein the included angle of the bamboo fibers in different layers is 0-3.5 degrees, and assembling the bamboo sheets into a blank with a layered structure;

(6) molding: hot-pressing the blank in the step (5) in a hot press, wherein the pressure is 40-120Mpa, the temperature is determined by the curing temperature of a reinforcing agent, the hot-pressing time is 70-150s/mm, and the blank is pressed into a laminated reinforcing plate with the thickness of 2.0-10.0 mm;

(7) nail blank processing: storing the laminated board in the step (6) for more than 4h at normal temperature or in a temperature and humidity regulating room, and cutting the laminated board into nail blanks according to the length and the size of each processed gun nail;

(8) machining: milling and grinding two surfaces of the nail blank of (7) according to the thickness specification of the gun nail to enable the nail head to be wedge-shaped, extruding the end surface of the nail tail to form deep marks parallel to the surface, wherein the number of the deep marks is positively correlated with the thickness of the nail body, the number of the deep marks is at least 1, the deep marks are positioned on the thickness central plane or the symmetrical plane of the end surface of the nail tail, the depth of the deep marks is 0.5-2mm, the depth of the deep marks in the middle of the thickness is deep, the depth of the deep marks closer to the two surfaces is shallow, and the taper angle of the deep marks is 10-40 degrees;

(9) and (3) wrapping end processing: wrapping one end of the nail tail of the nail body (8) with a compression-resistant resin layer, wherein the thickness of the resin layer is 0.9-2.8mm, extruding the two sides of the resin layer into a dovetail shape in a mold, and then curing the resin layer into a trapezoid, wherein the thickness of the long side of the nail tail end after curing is 1.5-2.0 times of the thickness of the nail body;

(10) stripping and arranging: and finally, quickly bonding the strip gun nails in rows in a lateral direction, wherein the bonding area is 5-25% of the area of the side surface, and manufacturing the strip bamboo gun nails.

Further, the bamboo age of the bamboo sections is 5 to 8 years.

Further, the thickness of the bamboo sheet is 0.12-0.25 mm.

Furthermore, the thickness of the nail body is less than 3mm and is 1, and the thickness of the nail body is more than 3mm and is 2-3.

Further, the compressive resin is selected from epoxy resin or modified isocyanate.

Further, the bamboo sheet is within 1/3 inner bamboo wall thickness near the outer bamboo green.

Furthermore, the automatic rotary differential sander is a toothpick sander with the positioning and sanding angles adjusted.

Further, the trapezoid angle of the trapezoid is 50-75 degrees.

The technical scheme provided by the embodiment of the application can have the following beneficial effects:

according to the embodiment, the thin slice obtained by rotary cutting the bamboo with the thickness of 0.12-0.25mm is used as the manufacturing unit, so that the thickness is thinner, and the longitudinal cracks are invisible to naked eyes on the back surface of the rotary cut thin slice, so that the problem that a bamboo chip reinforcer close to the green part of the bamboo is not easy to permeate is solved, the strength and the rigidity of the manufactured nail blank are effectively improved, the mechanical performance of the bamboo nail is improved, and the stability of the striking process of the bamboo nail is improved; because the moisture content of the bamboo chips after the first drying is controlled to be 3% -5%, the moisture content gradient in the dipping process is improved, the problem that the bamboo chip reinforcer close to the green part of the bamboo is difficult to permeate is further solved, and the adhesion amount of the reinforcer is effectively improved; the water content of the bamboo chips after the secondary drying is controlled to be 1-5%, so that the phenomena of bubbling and sliding sheets in the high-pressure high-temperature gluing forming process of the glued bamboo chips are overcome, and the yield and the production efficiency of the nail blank are improved; the included angles of the bamboo fibers at different layers in the assembly laminated structure are controlled to be 0-3.5 degrees, the condition that the tearing between the side surfaces starts to generate hair in the punching and cutting strip forming process is greatly reduced, the bamboo gun nail manufacturing method that the bamboo gun nails are punched and cut into strips and then adhered in rows is adopted, the problem of unevenness caused by the tearing of the side surfaces of the gun nails after the milling cutter is adopted for processing in the prior art is solved, and the problem of high requirement on the cutter grinding of the milling cutter used for milling the gun nails is also solved; the bamboo gun nail is pressed into a laminated reinforced plate with the thickness of 2.0-10.0mm by adopting the pressure of 40-120Mpa and the hot pressing time of 70-150s/mm, so that the mechanical property of a nail blank is improved, the stability of the bamboo nail after the gun nail is manufactured is improved, the bamboo gun nail is not only in the fields of traditional plate-type furniture, decoration and the like, but also can be expanded to be connected with components of a wood structure building, and the application range of the bamboo gun nail and the variety of the bamboo gun nail product are improved; carry out nail tail terminal surface and press the deep trace and wrap up the resin layer of resistance to compression and handle, overcome the problem that the bamboo nail had a hair after hitting among the original technology, both reduced the impact stress of bamboo rifle nail afterbody, increased the effective veneer area of resin layer and bamboo nail base, reduced the influence of possible impact unbalance loading to bamboo rifle nail stability, improved the post processing means by nail back work surface again.

It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the application.

Drawings

The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and together with the description, serve to explain the principles of the application.

Fig. 1 is a schematic view of a bamboo gun nail provided by an embodiment of the invention.

Fig. 2 is a schematic view of the bamboo gun nail in example 1, wherein the right end (tail) surface is square and the left end (head) is conical.

FIG. 3 is a schematic view of a bamboo gun nail according to example 2, wherein the right end (tail) surface is rectangular and the left end (head) is wedge-shaped … …

Fig. 4 is a schematic view of the bamboo gun nail in example 3, wherein the right end (tail) surface is square and the left end (head) is wedge-shaped.

The reference numerals in the figures are: nail head 1, nail body 2, nail tail 3, strengthening layer 4, thin bamboo sheet layer 5, deep mark 6, compressive resin layer 7, bamboo nail base 8.

Detailed Description

Reference will now be made in detail to the exemplary embodiments, examples of which are illustrated in the accompanying drawings. When the following description refers to the accompanying drawings, like numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present application. Rather, they are merely examples of apparatus and methods consistent with certain aspects of the present application, as detailed in the appended claims.

The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. As used in this application and the appended claims, the singular forms "a", "an", and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. It should also be understood that the term "and/or" as used herein refers to and encompasses any and all possible combinations of one or more of the associated listed items.

Example 1:

referring to fig. 1 and 2, the present embodiment provides a bamboo nailer, which is formed by a plurality of bamboo nails with equal thickness and width that are connected in parallel and adhered in a row, wherein a nail head 1 of the bamboo nail is in a wedge shape or a cone shape, and nail bodies of two adjacent bamboo nails2 are separated by adhesive, the thickness of the nail tail 3 of the bamboo nail is 1.5 times of the thickness of the nail body 2, the nail is square, the bamboo nail is a laminated structure with a strengthening layer 4 and thin bamboo sheet layers 5 which are separated one by one, and the density is 1310kg/m3

The production method of the bamboo gun nail can comprise the following steps:

(1) unit processing: and (3) rotatably cutting bamboo sections with the age of 7-8 years into bamboo sheets with the thickness of 0.13mm, wherein the bamboo sheets are positioned in the thickness of 1/3 inner bamboo walls close to the green of the bamboo.

(2) And (3) drying: drying the bamboo slices in the step (1) by adopting a hot pressing plate until the water content is 3%;

(3) strengthening: reinforcing the bamboo sheet in the step (2) by using a reinforcing agent of modified phenolic resin in an impregnation mode, wherein the solid content of the reinforcing agent is 10.5%, and the adhesion amount of the reinforcing agent is 25%; the modified phenol resin herein can be obtained from the 1688 market as long as it is known that the solid content of the reinforcing agent is 10.5% and the adhesion amount of the reinforcing agent is 25%.

(4) And (3) drying: drying the bamboo slices in the step (3) by adopting a pressing plate until the water content is 1.5-2.5%;

(5) assembling: superposing the bamboo sheets in the step (4) according to the same direction of the bamboo fibers, wherein the included angle of the bamboo fibers in different layers is 0-2 degrees, and assembling the bamboo sheets into a blank with a layered structure;

(6) molding: placing the blank in the step (5) in a hot press for hot pressing molding, wherein the pressure is 115Mpa, the temperature is 145 ℃, the hot pressing time is 150s/mm, and the blank is pressed into a laminated reinforced plate with the thickness of 9.5 mm;

(7) nail blank processing: storing the laminated board in the step (6) for 8 hours at normal temperature or in a temperature and humidity regulating room, and cutting the laminated board into nail blanks of 10cm according to the length size of the processed gun nails;

(8) machining: milling and grinding two surfaces of the nail blank in the step (7) according to the thickness specification of the gun nail to enable the nail head to be wedge-shaped, extruding the end surface of the nail tail to form deep marks parallel to the surface, wherein the number of the deep marks is 3, the positions of the deep marks are symmetrical to the thickness center of the end surface of the nail tail, the depth of the deep marks is 2mm and 1.2mm from the middle to the two surfaces respectively, and the cone angle of the deep marks is 35 degrees;

(9) and (3) wrapping end processing: wrapping one end of the nail tail in the step (8) with an EPO1551-310 epoxy resin layer to enable the thickness of the wrapped resin layer to reach 2.6mm, extruding two sides in a forming die to form a dovetail shape, and curing to form a trapezoid (the trapezoid angle is 70 degrees), wherein the thickness of the long edge of the nail tail end after curing is 1.5 times of the thickness of the nail body;

(10) stripping and arranging: and (2) rapidly punching and cutting the bamboo nails into strips according to the width of the bamboo nails, processing the strips into conical strips through an automatic rotary differential sander (the positioning and sanding angle is adjusted to be 30 degrees), and finally rapidly bonding the lateral thermoplastic adhesives of the strips into rows, wherein the bonding area is 6-8% of the area of the lateral surface, so as to prepare the rows of bamboo nails.

Example 2:

referring to fig. 3, in the present embodiment, a bamboo nail is provided, the bamboo nail is formed by a plurality of bamboo nails with equal thickness and width and adhered in parallel in a row, nail heads 1 of the bamboo nails are polygonal wedges, nail bodies 2 of two adjacent bamboo nails are separated by an adhesive, nail tails 3 of the bamboo nails are thicker than the nail bodies 2 and are respectively rectangular, the bamboo nails are layered structures with a reinforcing layer 4 and a thin bamboo sheet layer 5 at intervals, and the density is higher than 1280kg/m3

The production method of the bamboo gun nail is characterized by comprising the following steps:

(1) unit processing: and (3) rotatably cutting bamboo sections with the age of 5-6 years into bamboo sheets with the thickness of 0.18mm, wherein the bamboo sheets are positioned in the thickness of 1/4 inner bamboo walls close to the green of the bamboo.

(2) And (3) drying: drying the bamboo slices in the step (1) by adopting a hot pressing plate until the water content is 4% -5%;

(3) strengthening: selecting modified phenolic resin as a reinforcer, and performing reinforcement treatment on the bamboo sheet in the step (2) in an impregnation mode, wherein the solid content of the reinforcer is 15%, and the adhesion amount of the reinforcer is 23% -25%; the modified phenolic resin herein can be obtained from 1688 as long as it is known that the reinforcing agent has a solids content of 15% and a reinforcing agent adhesion amount of 23% to 25%.

(4) And (3) drying: drying the bamboo slices in the step (3) by adopting a hot pressing plate until the water content is 2% -3.5%;

(5) assembling: superposing the bamboo sheets in the step (4) according to the same direction of the bamboo fibers, wherein the included angle of the bamboo fibers in different layers is 0-3 degrees, and assembling the bamboo sheets into a blank with a layered structure;

(6) molding: placing the blank in the step (5) in a hot press for hot pressing molding, wherein the pressure is 95Mpa, the temperature is 135-140 ℃, the hot pressing time is 80s/mm, and the laminated reinforced plate with the thickness of 2.0mm is pressed;

(7) nail blank processing: storing the laminated board in the step (6) for 4.5h at normal temperature or in a temperature and humidity regulating room, and cutting the laminated board into 22mm nail blanks according to the length size of the processed gun nails;

(8) machining: milling and grinding two surfaces of the nail blank in the step (7) according to the thickness specification of the gun nail to enable the nail head to be wedge-shaped, extruding the end face of the nail tail to form deep marks parallel to the surface, wherein the number of the deep marks is 1, the deep marks are positioned in the thickness center of the end face of the nail tail, the depth is 0.5mm, and the cone angle of the deep marks is 15 degrees;

(9) and (3) wrapping end processing: wrapping one end of the nail tail in the step (8) with an Epo1551-310 epoxy resin layer, controlling the thickness of the resin layer to be 0.9mm, extruding two sides of the nail tail in a forming die to form a dovetail shape, curing to form a trapezoid (the trapezoid angle is 50 degrees), and enabling the thickness of the long edge of the nail tail end to be 2.0 times of the thickness of the nail body after curing;

(10) stripping and arranging: and (3) rapidly punching and cutting the bamboo nails into strips according to the width of each bamboo nail, and rapidly bonding the strips of bamboo nails into rows in the lateral direction, wherein the bonding area is 10-15% of the area of the side surface, so as to prepare the rows of bamboo nails.

Example 3:

referring to fig. 4, the present embodiment provides a bamboo nailing gun, the bamboo nailing gun is formed by a plurality of bamboo nails with equal thickness and width, which are connected in parallel and adhered in rows, nail heads 1 of the bamboo nails are wedge-shaped, two adjacent bamboo nails are separated by an adhesive between nail bodies 2, nail tails 3 of the bamboo nails are thicker than the nail bodies 2 and are respectively square, the bamboo nails are layered structures with a reinforced layer 4 and a thin bamboo sheet layer 5, and the density is 1210kg/m3

The production method of the bamboo gun nail is characterized by comprising the following steps:

(1) unit processing: and (3) rotatably cutting bamboo sections with the age of 6-7 years into bamboo sheets with the thickness of 0.22mm, wherein the bamboo sheets are positioned in the thickness of 1/3 inner bamboo walls close to the green of the bamboo.

(2) And (3) drying: drying the bamboo slices in the step (1) by adopting a hot pressing plate until the water content is 4% -5%;

(3) strengthening: selecting modified melamine resin as a reinforcer, and performing reinforcement treatment on the bamboo sheet in the step (2) in an impregnation mode, wherein the solid content of the reinforcer is 12-13%, and the adhesion amount of the reinforcer is 22-23%; it should be noted that the modified melamine resin can be obtained from 1688 as long as it is known that the solid content of the reinforcing agent is 12% to 13% and the adhesion amount of the reinforcing agent is 22% to 23%.

(4) And (3) drying: drying the bamboo slices in the step (3) by adopting a hot pressing plate until the water content is 3% -4%;

(5) assembling: superposing the bamboo sheets in the step (4) according to the same direction of the bamboo fibers, wherein the included angle of the bamboo fibers in different layers is 0-3.5 degrees, and assembling the bamboo sheets into a blank with a layered structure;

(6) molding: placing the blank in the step (5) in a hot press for hot pressing molding, wherein the pressure is 50Mpa, the temperature is 135 ℃, the hot pressing time is 70s/mm, and the blank is pressed into a laminated reinforced plate with the thickness of 4.0 mm;

(7) nail blank processing: storing the laminated board in the step (6) for 6h at normal temperature or in a temperature and humidity regulating room, and cutting the laminated board into 32mm nail blanks according to the length size of the processed gun nails;

(8) machining: milling and grinding two surfaces of the nail blank in the step (7) according to the thickness specification of the gun nail to enable the nail head to be wedge-shaped, extruding the end face of the nail tail to form deep marks parallel to the surface, wherein the number of the deep marks is 2, the positions of the deep marks are symmetrical to the thickness center of the end face of the nail tail, the depth of the deep marks is 1mm, and the taper angle of the deep marks is 25 degrees;

(9) and (3) wrapping end processing: wrapping one end of the nail tail (8) with a compression-resistant modified isocyanate resin layer, controlling the thickness of the resin layer to be 1.8mm, extruding two sides of the resin layer into a dovetail shape in a forming die, and curing the resin layer into a trapezoid (the trapezoid angle is 50), wherein the thickness of the long edge of the nail tail end after curing is 2 times of that of the nail body;

(10) stripping and arranging: and (3) rapidly punching and cutting the bamboo nails into strips according to the width of each bamboo nail, and rapidly bonding the strips of bamboo nails into rows in the lateral direction, wherein the bonding area is 10-20% of the area of the side surface, so as to prepare the rows of bamboo nails.

The bamboo gun nail produced in the embodiment 1 is mainly used for connecting medium and large wood structures, such as nailing of modern wood structure building components and nailing of large wood boards, table legs and shelves; the bamboo gun nail produced in example 2 is mainly used for nailing indoor wood decoration materials and nailing components of products such as general wood (plate type) furniture, wood composite doors, cabinets and the like. The bamboo gun nail produced in the example 3 is mainly used for nailing between wood or artificial board components with low density.

According to the bamboo gun nail obtained through the embodiment, the yield of the production process is improved to more than 99%, the situations of nail tail fluffing, tearing between nails and the like do not occur in the using process, and if hard knots are not touched in the striking process, the stability of the bamboo nail is obviously improved.

Other embodiments of the present application will be apparent to those skilled in the art from consideration of the specification and practice of the disclosure disclosed herein. This application is intended to cover any variations, uses, or adaptations of the invention following, in general, the principles of the application and including such departures from the present disclosure as come within known or customary practice within the art to which the invention pertains. It is intended that the specification and examples be considered as exemplary only, with a true scope and spirit of the application being indicated by the following claims.

It will be understood that the present application is not limited to the precise arrangements described above and shown in the drawings and that various modifications and changes may be made without departing from the scope thereof. The scope of the application is limited only by the appended claims.

11页详细技术资料下载
上一篇:一种医用注射器针头装配设备
下一篇:一种竹木静音门加工制作系统

网友询问留言

已有0条留言

还没有人留言评论。精彩留言会获得点赞!